AlloyRef. No.Ag
ColourDensity
g/cm³
Melting range
°C
Hardness
supplied HV5
Pre-heating temperature
°C
Casting temperature
°C

Au 333 112-333 45 red 10.8 935 – 1000 110 approx. 600 1100 – 1200
PDF
Au 333 650-333 90 yellow 10.6 820 – 910 110 approx. 600 1010 – 1110
PDF
Au 333-Ag 655-333 580 white 12.1 840 – 915 115 approx. 600 1015 – 1115
PDF










Au 585 115-585 70 bright red 12.9 870 – 940 140 approx. 600 1040 – 1140
PDF
Au 585 127-585 335 yellow ON
14.0 870 – 890 125 approx. 600 990 – 1090
PDF
Au 585-Pd 10 134-585 280 white 14.4 1055 – 1150 100 approx. 650 1250 – 1350
PDF










Au 750 609-750 50 bright red 15.1 860 – 900 165 approx. 600 1000 – 1100
PDF
Au 750 156-750 125 rich yellow 3N 15.4 890 – 915 150 approx. 600 1015 – 1115
PDF
Au 750 122-750 150 yellow 2N 15.5 855 – 900 140 approx. 600 1000 – 1100
PDF
Au 750-Pd 10 126-750 100 white 15.9 1040 – 1130 110 approx. 650 1230 – 1330
PDF










Ag 935 420-935 935 white 10.3 825 – 900 65 approx. 600 1000 – 1100
PDF
Ag 935 PAT II 441-935 935 white 10.3 830 – 910 60 approx. 600 1010 – 1110
PDF










Pt 950 177-950 0 white 20.2 1730 – 1740 135 approx. 1000 1840 – 1940
PDF