| Copper/silver alloys |
| Ref. No. | Alloy | Density [g/cm³] | Melting range [°C] | Electrical conductivity [m/Ωmm²] | Electrical resistance [µΩm] | Electrical elasticity [GPa] | Tensile strength** [Mpa] | Vickers hardness ** [ HV] |
±10%
| ±10%
| ±20%
|
| soft | hard | soft | hard |
| 454 – 001 |
CuAg 0,1 |
8,9 |
1080 |
56 |
0,02 |
110 |
200 |
360 |
45 |
120 |
| 450 – 010 |
CuAg 1 |
8,9 |
1065 – 1080 |
53 |
0,02 |
125 |
260 |
500 |
50 |
150 |
| 451 – 020 |
CuAg 2 |
9 |
1050 – 1075 |
49 |
0,02 |
123 |
280 |
530 |
60 |
160 |
| 452 – 030 |
CuAg 3 |
9,1 |
1035 - 1070 |
47 |
0,02 |
122 |
300 |
550 |
65 |
170 |
| 456 – 060 |
CuAg 6 |
9,2 |
960 - 1050 |
45 |
0,03 |
120 |
320 |
580 |
70 |
180
|
Further materials on request.
** Other values available on request.
| Silver/gold alloys |
| Ref. No. | Alloy | Density [g/cm³] | Melting range [°C] | Electrical conductivity [m/Ωmm²] | Electrical resistance [µΩm] | Electrical elasticity [GPa] | Tensile strength** [Mpa] | Vickers hardness ** [ HV] |
±10%
| ±10%
| ±20%
|
| soft | hard | soft | hard |
| 400 – 998 |
AgAu 0,2 |
10,5 |
960 |
60 |
0,0167 |
80 |
200 |
380 |
45 |
110 |
| 400 – 982 |
AgAu 1,8 |
10,5 |
962 – 965 |
58 |
0,0175 |
81 |
210 |
410 |
50 |
120 |
| 400 – 975 |
AgAu 2,5 |
10,6 |
963 – 967 |
58 |
0,0172 |
81 |
210 |
415 |
50 |
125 |
| 400 – 950 |
AgAu 5 |
10,7 |
965 - 970 |
57 |
0,02 |
85 |
220 |
420 |
55 |
125 |
| 400 – 900 |
AgAu 10 |
10,9 |
965 - 975 |
57 |
0,02 |
85 |
220 |
440 |
65 |
130
|